Wave Soldering TroubleshootingWhen these defects occur, check the flux and conveyor speed.

Last month, we discussed insufficient solder topside fillets. This month, we look at insufficient solder bottom-side fillets (Figure 1). Per IPC-A-610, an acceptable condition is a 100% solder fillet and circumferential wetting present on the secondary (solder source) side of the solder joint. The minimum acceptable condition is a 330° circumferential fillet and wetting present for Class 3 boards, and 270° for Class 1 and 2 boards.
Fig. 1

Primary process setup areas to check are:

  • Conveyor speed too slow.
  • Excessive time over preheat, causing the flux to be burned off.
  • Excessive dwell time, causing flux to be destroyed before exiting the wave.
  • Excessive bottom-side board temperature, causing flux to be burned off before the wave.
  • Insufficient flux or flux activity.
  • Wave height too low on one or both waves.
Other things to look for in the process:
  • Insufficient solder temperature.    
  • Excessive preheat.    
  • Excess flux blow-off.
  • Board not seated properly.    
  • Insufficient preheat.    
  • Insufficient flux blow-off.
  • Solder wave height too low.    
  • Contaminated flux.    
  • Flux not making contact.
  • Solder wave uneven.    
  • Flux SP GR too low.    
  • Conveyor speed high.
  • Solder contaminated.    
  • Flux SP GR too high.     
  • Flux applied unevenly.    

    
Other things to look for with the assembly:     

  • Board contamination.    
  • Improper board handling.    
  • Component contamination.
  • Component leads too short.
Other things to look for with the bare board:
  • Board oxidized.    
  • Mask in hole.     
  • Board warped.    
  • Board contaminated.    
  • Poor plating in the hole.    
  • Component contamination.
  • Misregistration of the mask.    
  • Hole and pad misregistered.

Other things to look for with the board design:

  • Poor pallet design.    
  • Internal ground plane.    
  • Pad size mismatched.
  • Large ground plane on component side.
  • Lead-to-hole ratio too large.     
  • Weight distribution.
  • Large ground plane on solder side.

Paul Lotosky is global director - customer technical support at Cookson Electronics (cooksonelectronics.com) This e-mail address is being protected from spambots. You need JavaScript enabled to view it .


blog comments powered by Disqus
Last Updated on Tuesday, 02 June 2009 20:16
 

Columns

European RoHS Enforcement Explained

A series of workshops next month on compliance with RoHS and other directives will help US companies looking to break into the European market.

Read more...
 
Believing Foxconn Means Suspending Belief

The Foxconn makeover is in full swing, with the latest this piece from the New York Times that supposes that the world's largest ODM is worried that Apple -- yes, Apple -- might be bringing it down:

Read more...
 

Features

Managing Your ESD Program

The processes are as important as the tools.

Read more...
 
SMT Reflow Oven-to-Oven Repeatability

How to adjust an oven so a single recipe will work across multiple ovens for an individual product.

Read more...
 

Search

Search

Login

CB Login

Language

Language

English French German Italian Portuguese Russian Spanish
 

Products

Polyonics Introduces Double Coated Bonding Tapes
Ultra thin double coated tapes are for bonding and attaching components and assemblies where high dielectric strength is required. REACH and RoHS compatible. Come in polyimide (PI) and polyester...